Mesh fabric dyeing and finishing: flowcharts for polyester, cotton and CVC mesh

Mesh fabric dyeing and finishing flowcharts for polyester, cotton and CVC mesh: when to heat set, holding GSM on an open knit, faults and real data.

Mesh fabric dyeing and finishing: flowcharts for polyester, cotton and CVC mesh

Mesh is the open, breathable knit of sportswear, and in our records two out of three mesh parts are 100% polyester. Here is the dyeing and finishing route for each fibre, from greige mesh to the cutting table.

At a glance

76Parts in our records

180Median required GSM

19%Within GSM tolerance

76%Polyester mesh heat set

Mesh is a knit with a regular pattern of open holes, made with tuck stitches or needle transfers. Plain mesh, micro mesh, spider mesh and design mesh differ in the size and shape of the holes. It is light and breathable, which is why most of it goes into sportswear and linings.

Type in our recordsParts
Mesh51
Design Mesh10
Spider Mesh5
D.Mesh3
Micro Mesh3
Y/D Mesh2
Ly Mesh1
Ly Spider Mesh1

By fibre: what our records show

Fibre or blendPartsMedian required GSMWithin ±5% GSMMore than 5% lightMedian length shrinkageMedian width shrinkageHeat set
Polyester5115018%69%3%2%76%
100% cotton1522020%33%7%7%20%
CVC / PC621017%33%2%2%100%

Polyester mesh makes up 51 of 76 mesh parts. Only 18% of it finishes within GSM tolerance, and 76% is heat set.

Our records hold fewer parts of this fabric than of the common knits, so read the figures as a guide, not a rule.

When mesh is heat set

  • 100% polyester mesh is heat set, 99 times out of 100. We skip it only for a special buyer requirement or for swatch development.
  • Mesh made from yarn-dyed polyester is not heat set.
  • Most cotton mesh is not heat set.

Holding mesh GSM

  • Mesh is a loose, open design, so GSM is hard to hold within tolerance.
  • For polyester mesh we control GSM through heat setting, or we discuss the GSM with the buyer.
  • Polyester mesh does not need a wash test for GSM. Cotton mesh does: we check its GSM after washing.

The sequence before the dyeing machine

Every chart below follows the same sequence before dyeing. Steps a fabric does not need simply drop out; they are drawn dashed.

  1. Greige inspection, then batching. A fabric that stays a tube is turned inside out here.
  2. If it needs heat setting, singeing or mercerising: slitting first. None of these is ever done on a tube.
  3. If it needs heat setting: heat setting in open width.
  4. If it needs singeing: singeing in open width, after checking the flame cannot damage the fabric.
  5. If it is mercerised: mercerising, then drying.
  6. If the fabric was opened: back sewing, to make it a tube again with the face side inside (the loop side, for terry).
  7. Loading into the dyeing machine, then scouring, bleaching and dyeing, single part or double part as the fibre needs.

Flowcharts by fibre

Polyester mesh fabric

In our records: 51 parts, 18% within GSM tolerance, median length shrinkage 3%, heat set 76%. Full process: Polyester dyeing process.

Dyeing and finishing: Polyester mesh fabric

Start: greige mesh fabricfrom knitting
Greige inspectionholes, yarn faults, GSM
Batchingone lot per batch; turned inside out if it stays a tube
Slittingopen width: never heat set, singed or mercerised as a tube
Heat settingopen, 180–190°C
Back sewinginto a tube, face side inside
Load in dyeing machine
Disperse dyeing130°C; load at 80°C
Reduction clearingevery shade
Softener
Slittingopen width
Stenter100–110°C when polyester is dyed
Compactingshrinkage
Final inspectionGSM, shrinkage, shade
End: finished rollto cutting
GreigePreparationDyeingAfter-treatmentFinishing
Flow chart: Polyester mesh fabric, from greige fabric to the cutting table. Dashed steps run only when needed.

100% cotton mesh fabric

In our records: 15 parts, 20% within GSM tolerance, median length shrinkage 7%, heat set 20%. Full process: 100% cotton dyeing process.

Dyeing and finishing: 100% cotton mesh fabric

Start: greige mesh fabricfrom knitting
Greige inspectionholes, yarn faults, GSM
Batchingone lot per batch; turned inside out if it stays a tube
Slittingopen width: never heat set, singed or mercerised as a tube
Heat settingopen, 180–190°C; if elastane, tight or design
Singeingopen width; when no enzyme can be used and a clean face is needed; never on polyester faces
Back sewinginto a tube, face side inside
Load in dyeing machine
Scour-bleach98°C × 60 min; heavy: 70–80°C
Enzymebio-polish
Reactive dyeing60°C
Wash-off & soaping
Fixing & softener
Slittingopen width
Stenterabout 150°C; width, GSM
Compactingshrinkage
Final inspectionGSM and shrinkage after wash, shade
End: finished rollto cutting
GreigePreparationDyeingAfter-treatmentFinishingOnly when needed
Flow chart: 100% cotton mesh fabric, from greige fabric to the cutting table. Dashed steps run only when needed.

CVC / PC mesh fabric

In our records: 6 parts, 17% within GSM tolerance, median length shrinkage 2%, heat set 100%. Full process: CVC / PC dyeing process.

Dyeing and finishing: CVC / PC mesh fabric

Start: greige mesh fabricfrom knitting
Greige inspectionholes, yarn faults, GSM
Batchingone lot per batch; turned inside out if it stays a tube
Slittingopen width: never heat set, singed or mercerised as a tube
Heat settingopen, 180–190°C; if PC, elastane, tight or design
Singeingopen width; when no enzyme can be used and a clean face is needed; never on polyester faces
Back sewinginto a tube, face side inside
Load in dyeing machine
Polyester dyeingdisperse, 130°C
Reduction clearing80°C × 10 min
Scouring98°C × 60 min
Enzymecotton part
Cotton dyeingreactive, 60°C
Soaping & softener
Slittingopen width
Stenter100–110°C when polyester is dyed
Compactingshrinkage
Final inspectionGSM, shrinkage, shade
End: finished rollto cutting
GreigePreparationDyeingAfter-treatmentFinishingOnly when needed
Flow chart: CVC / PC mesh fabric, from greige fabric to the cutting table. Dashed steps run only when needed.

Common faults and buyer complaints

Mesh faults follow from its open structure.

Holes distorted or width off. The open structure pulls out of shape easily. Fix the width at heat setting and hold the same width on the stenter, without overstretching.

GSM out of tolerance. Set GSM through heat-setting width and overfeed on polyester mesh, check cotton mesh after washing, and agree the GSM with the buyer before bulk when the design makes it hard.

Crease marks on polyester mesh. Heat set before dyeing and load the fabric straight; polyester creases set hard at 130°C.

Kamrul Islam
Kamrul Islam

Textile engineer with 14+ years in dyeing and fabric development. He writes every guide on Dyeing Solution from real production work. Full profile